| Ryton® R-4-220 PPS is an advanced 40% fiberglass reinforced polyphenylene sulfide compound formulated for enhanced hydrolytic stability in applications requiring constant or repeated exposure to high temperature water. |
|
| Nominal Engineering Properties(1) |
R-4-220NA |
R-4-220BL |
Test Method |
| Tensile Strength, Ksi |
28.0 |
26.0 |
ASTM D638 |
| Elongation, % |
1.6 |
1.5 |
ASTM D638 |
| Flexural Strength, Ksi |
39.0 |
36.0 |
ASTM D790 |
| Flexural Modulus, Msi |
2.1 |
2.1 |
ASTM D790 |
| Notched Izod Impact, ft·lb/in, 1/8 in specimen |
1.6 |
1.4 |
ASTM D256 |
| Unnotched Izod Impact, ft·lb/in, 1/8 in specimen |
12.0 |
10.0 |
ASTM D256 |
| Compressive Strength, Ksi |
39.0 |
39.0 |
ASTM D695 |
| Heat Deflection Temperature 264 psi,°F(2) |
>500 |
>500 |
ASTM D648 |
| UL Temperature Index,°C |
200 / 220 |
200 / 220 |
UL 746B |
| Coefficient of Linear Thermal Exp., X 10-6 in/in/°C |
  |
  |
ASTM E831 |
| Axial Direction, -50°C to 50°C |
15 |
15 |
  |
| Axial Direction, 100°C to 200°C |
15 |
15 |
  |
| Transverse Direction, -50°C to 50°C |
40 |
40 |
  |
| Transverse Direction, 100°C to 200°C |
90 |
90 |
  |
| Flammability Rating |
V-0 |
V-0 |
UL 94 |
| Thermal Conductivity, BTU·in/hr·ft2·°F |
2.1 |
2.1 |
  |
| Dielectric Strength, V/mil |
550 |
550 |
ASTM D149 |
| Dielectric Constant, 78° F |
|
|
ASTM D150 |
| 1kHz |
3.8 |
3.8 |
  |
| 1MHz |
3.8 |
3.8 |
  |
| Dissipation Factor, 78°F |
|
|
ASTM D150 |
| 1 kHz |
0.002 |
0.002 |
|
| 1 MHz |
0.003 |
0.003 |
|
| Volume Resistivity, ohm·cm |
1 x 1016 |
1 x 1016 |
ASTM D257 |
| Arc Resistance, sec |
125 |
125 |
ASTM D495 |
| Comparative Tracking Index, V |
150 |
150 |
UL 746A |
| Mold Shrinkage(3) in/in, Flow/Transverse |
0.003 / 0.005 |
0.003 / 0.005 |
  |
| Density, g/cc |
1.68 |
1.68 |
ASTM D792 |
| Water Absorption, % |
0.02 |
0.02 |
ASTM D570 |
| Color |
Natural |
Black |
  |
| Hydrolytic Stability(4) |
  |
  |
  |
| Tensile Strength Retained, % |
>80 |
>80 |
  |
| Weight Gain, % |
<1.0 |
<1.0 |
  |
|
| (1) Test specimen molding conditions: Stock Temperature, 600-650° F; Mold Temperature, 275° F |
| (2) Annealed 2 hours at 400° F |
| (3) Measured on 4 in X 4 in X 1/8 in Plaques, Edge Gated |
| (4) Test specimens aged 1000 hours in water at 140° C (284° F) |
| The nominal properties reported herein are typical of the product but do not reflect normal testing variances and therefore should not be used for specification purposes. |
| Ryton® R-4-220 PPS is an advanced 40% fiberglass reinforced polyphenylene sulfide compound formulated for enhanced hydrolytic stability in applications requiring constant or repeated exposure to high temperature water. |
|
| Nominal Engineering Properties(5) |
R-4-220NA |
R-4-220BL |
Method |
| Tensile Strength, MPa |
190 |
175 |
ISO 527 |
| Elongation, % |
1.6 |
1.4 |
ISO 527 |
| Flexural Strength, MPa |
270 |
250 |
ISO 178 |
| Flexural Modulus, GPa |
14 |
14 |
ISO 178 |
| Notched Izod Impact, kJ/m2 |
9.0 |
8.0 |
ISO 180A |
| Unnotched Izod Impact, kJ/m2 |
35 |
30 |
ISO 180A |
| Compressive Strength, MPa |
265 |
265 |
ISO 604 |
| Heat Deflection Temperature 1.8 MPa,°C(6) |
>260 |
>260 |
ISO 75 |
| UL Temperature Index,°C |
200 / 220 |
200 / 220 |
UL 746B |
| Coefficient of Linear Thermal Exp., X 10-6 m/m/°C |
  |
  |
ISO 11359-2 |
| Axial Direction, -50°C to 50°C |
15 |
15 |
|
| Axial Direction, 100°C to 200°C |
15 |
15 |
|
| Transverse Direction, -50°C to 50°C |
40 |
40 |
|
| Transverse Direction, 100°C to 200°C |
90 |
90 |
  |
| Flammability Rating |
V-0 |
V-0 |
UL 94 |
| Thermal Conductivity, W/m·K |
0.31 |
0.31 |
  |
| Dielectric Strength, kV/mm |
22 |
22 |
ASTM D149 |
| Dielectric Constant, 25°C |
|
|
ASTM D150 |
| 1kHz |
3.8 |
3.8 |
|
| 1MHz |
3.8 |
3.8 |
|
| Dissipation Factor, 25°C |
  |
|
ASTM D150 |
| 1 kHz |
0.002 |
0.002 |
|
| 1 MHz |
0.003 |
0.003 |
|
| Volume Resistivity, ohm·cm |
1 x 1016 |
1 x 1016 |
ASTM D257 |
| Arc Resistance, sec |
125 |
125 |
ASTM D495 |
| Comparative Tracking Index, V |
150 |
150 |
UL 746A |
| Insulation Resistance, ohm (90°C, 95% RH, 48 hr) |
1 x 1012 |
1 x 1012 |
|
| Mold Shrinkage(7) m/m, Flow/Transverse |
0.003 / 0.005 |
0.003 / 0.005 |
  |
| Density, g/cc |
1.68 |
1.68 |
ISO 1183A |
| Water Absorption, % |
0.02 |
0.02 |
ASTM D570 |
| Color |
Natural |
Black |
  |
| Hydrolytic Stability(8) |
  |
  |
  |
| Tensile Strength Retained, % |
>80 |
>80 |
  |
| Weight Gain, % |
<1.0 |
<1.0 |
  |
|
| (5) Test specimen molding conditions: Stock Temperature, 314-345° C; Mold Temperature, 135° C. |
| (6) Annealed 2 hours at 200° C |
| (7) Measured on 102 mm X 102 mm X 3.2 mm Plaques, Edge Gated |
| (8) Test specimens aged 1000 hours in water at 140° C |
| The nominal properties reported herein are typical of the product but do not reflect normal testing variances and therefore should not be used for specification purposes. |
|
|